Hot Dip Galvanizing Service

Seen Steel arranges hot dip galvanizing for fabricated steel across the UAE. You send the finished fabrication in black steel, it goes through the bath, and it comes back coated to EN ISO 1461. This is for work that has already been cut, welded and drilled, where painting will not last long enough in this climate.

What size goes in

Single pieces up to 14 metres long and 4 metres high go through in one dip. That takes a full 12 metre length with room to spare, and covers most fabricated frames, trusses, ladders, handrail runs and structural assemblies without cutting anything down to fit.

Anything longer than that has to be either split at a bolted joint or progressively dipped, and progressive dipping leaves a visible line where the two immersions meet. Send the overall length early and we will tell you which way your item has to go, because it is far cheaper to design a joint in than to discover the problem once the steel is welded.

Why hot dip rather than paint

Hot dip galvanizing is not a coating sitting on the surface. The steel is dipped in molten zinc, and the zinc reacts with the iron to form alloy layers that are part of the steel itself. That is why it survives handling, bolting and site knocks that would chip paint, and why it keeps protecting at a cut edge or a scratch, where the surrounding zinc sacrifices itself to shield the exposed steel.

In the UAE the deciding factor is usually salt. Anything outdoors within reach of coastal air, which covers most of the country, corrodes painted steel far faster than inland work. Galvanizing is normally the cheaper answer once you count the repaint cycles you avoid.

Years to first maintenance for hot dip galvanized steel in UAE conditions, compared with a painted steel system

What happens to your steel

Degreasing and abrasive blasting first, to take off oil, dirt and loose scale. Then acid pickling, which strips the remaining mill scale and rust back to clean bare steel. Then fluxing and drying, because a wet piece entering molten zinc is dangerous. Then the dip itself at 445 to 455 degrees, held long enough for the alloy layers to grow. Then cooling and inspection against the standard.

The blasting and pickling stages are why work comes back with an even finish instead of patches, and they are also why paint, lacquer and heavy weld spatter have to be removed beforehand. Those survive the acid and leave bare spots underneath.

The nine stages of a hot dip galvanizing line, from degreasing through the zinc kettle to inspection

Coating thickness to EN ISO 1461

The thickness of the coating is set by the thickness of the steel, not by what anyone asks for. Thicker steel holds the zinc longer in the bath and grows a heavier layer. These are the minimums the standard requires for articles that are not centrifuged:

Steel thickness Local minimum Mean minimum
6 mm and over 70 microns 85 microns
3 mm up to 6 mm 55 microns 70 microns
1.5 mm up to 3 mm 45 microns 55 microns
Under 1.5 mm 35 microns 45 microns

If your specification calls for ASTM A123 instead, say so on the enquiry. The two standards are close but the thickness bands and the test method differ, and a consultant who asked for one will not accept a certificate for the other.

Cross section of a hot dip galvanized coating showing the eta, zeta, delta and gamma zinc iron alloy layers on steel

Preparing work for the bath

Most galvanizing problems start at the fabrication stage rather than at the plant, and they are all avoidable.

  • Vent and drain holes. Every sealed section needs a way for air to escape and for zinc to run out. A hollow section or a closed box with no holes will either float, trap air and go uncoated inside, or build pressure in the bath. This is the single most common reason work gets sent back.
  • No fully sealed voids. Anything completely closed is a safety risk in the bath. If a void cannot be vented, it has to be redesigned or left out of the dip.
  • Overlaps and faying surfaces. Where two plates lap without being seal welded, acid gets in during pickling and bleeds back out afterwards, staining the coating. Either seal weld the overlap or leave a gap wide enough to drain.
  • Surface condition. Paint, grease, weld slag, lacquer markings and heavy mill scale do not pickle off and will leave bare patches. Clean the work before it goes.
  • Distortion. Thin sheet, long slender members and welds concentrated on one side can pull when the steel heats up. Balance welding where you can and tell us if a piece has tight tolerances to hold.

Correct vent and drain hole positions on closed hollow steel sections for hot dip galvanizing

What to send for a quotation

Galvanizing is quoted on the weight of steel going through the bath, so the figures we need are:

  • Total weight of the batch
  • The size of the largest single piece, length, width and height
  • The thinnest material in the batch, which sets the coating class
  • Number of pieces, and whether they are all the same
  • The standard called for, EN ISO 1461 or ASTM A123
  • A drawing or photograph if the shape is awkward

Send that through the enquiry form or on WhatsApp at +971 56 227 5722 and we come back with a rate and a turnaround. If you are not sure of the weight, the product pages carry kilograms per metre for every section we supply, which is usually enough to work it out.

Already galvanized material, no service needed

If you have not fabricated anything yet and simply want material that arrives coated, buy it that way instead. It costs less than galvanizing afterwards and there is no second handling. We supply galvanized square hollow section, galvanized rectangular hollow section, galvanized round pipes, GI gratings, and GI coil and sheet in zinc classes Z120 through Z275.

The choice usually comes down to whether the steel gets cut after coating. Cut a galvanized tube and the cut end is bare, which is fine for indoor work and not fine on the coast. Fabricate first and galvanize after and every surface is covered, welds included.